1708 Usage

cmperry56

Seaman
Joined
Aug 19, 2010
Messages
51
I have a quick question about using biaxial 1708 on stringers. Since 1708 has a layer of CSM on one side, which side should be laid against the form material?
 

zool

Captain
Joined
Aug 19, 2012
Messages
3,433
Re: 1708 Usage

You lay it mat (08) side down, it blends with the styrene in the poly resin to form the bond on the substrate...
 

jigngrub

Fleet Admiral
Joined
Mar 19, 2011
Messages
8,155
Re: 1708 Usage

Yeah, CSM side to the wood for that nice cloth look on top when it's wet out.
 

cmperry56

Seaman
Joined
Aug 19, 2010
Messages
51
Re: 1708 Usage

Thanks to all. I thought that was the way to go but I couldn't find anything that said specifically.
 